Two-part high-temperature investment
FERROVEST™V.H.T.
For platinum, palladium
and stainless steel.
A matched powder-and-binder system for demanding alloys, including metals melting above 1500°C. Developed for smooth surfaces and dependable results at high casting temperatures.
- 22.5 kg Poly sack
- 22.5 kg Ergonomic plastic drum
- 45 kg Plastic box
Supplied with enough binder concentrate to process the entire powder quantity. The heavy-duty plastic drums can also be used to contain spent investment.
01 / The FERRO VEST V.H.T. difference
High temperatures.
Fine surfaces.
FERRO VEST V.H.T. is a two-part investment developed for platinum, palladium, stainless steel and other metals melting above 1500°C. Its matching concentrate must be diluted before mixing with the powder.
A system designed to work together.
Consistent flow. Cleaner detail.
Less finishing after casting.
POWDER + MATCHED BINDER
Measure carefully.
Prepare for strength.
Diluted binder solution · 28–30 mL/100 g
Enter 0.001–10,000 kg of dry powder.
Binder concentrate L
Distilled water L
Total diluted solution L
Acidic binder: wear protective glasses and gloves. Carefully add concentrate to water. The center may settle about 1″ (2.54 cm); maintain at least 2″ (5.08 cm) of cover above the patterns. Curing takes a few hours to overnight, depending on flask size.
Calculation details
All results are volumes in liters, not weights.
1 L = 1,000 ml. Results rounded to 6 decimal places.
Binder = total solution ÷ 20
Distilled water = total solution × 19 ÷ 20
- 01 · 1 : 19
Prepare the binder
Measure the powder. Carefully add 1 part concentrate to 19 parts distilled water by volume. Use the calculator to measure the required solution.
- 02 · 10–15 MIN
Add gradually, then mix
Use a heavy-duty, high-torque mixer. Add powder slowly at low speed, letting each addition thin. After all powder is added, mix at medium speed for a further 10–15 minutes.
- 03 · +2 MIN
Vacuum the slurry
Apply full vacuum until the slurry rises, breaks and begins to boil. Continue under vacuum for 2 minutes.
- 04 · ≥ 5.08 CM
Fill along the flask wall
Pour gently down the inside wall, avoiding the patterns. Cover the top row with at least 2″ (5.08 cm) of investment.
- 05 · 2 MIN
Vacuum filled flasks
Vacuum the filled flasks for 2 minutes.
- 06 · HOURS / OVERNIGHT
Leave to cure
Leave undisturbed until a thick, dull gray paste forms. Cure on newspaper; with rubber bases, use a 3″ (7.62 cm) bed of unused FERRO VEST V.H.T. powder.
- 07 · +2 HOURS
Remove rubber bases
After the investment appears hard, wait two additional hours before carefully removing a rubber base.
Prepare the flask & sprue base
Provide a path for excess binder moisture to wick away.
Flasks up to 3″ × 3″
Use a permeable cellulose-paper base 1/16″ (1.588 mm) thick and 4″ (10.16 cm) wide, with a 0.75″ (1.905 cm) drainage hole. Alternatively use three automatic-drip coffee filters or suitable permeable paper with the same hole, securing raised edges with strong rubber bands.
Attach a pre-made wax button using sticky wax, then the sprue rod.
Line the flask Use non-asbestos cellulose paper cut 1″ (2.54 cm) shorter than the flask, with equal gaps at top and bottom.
Add masking tape or a removable rubber extension at the top for vacuuming.
Larger flasks with rubber basesCut holes around the sprue button. Place cotton cloth around it, center the flask and press firmly into the cloth and base. Alternatively remove the rubber cone and seal a pre-made wax button to the cloth. Use a top collar or tape for vacuuming.
Watch the preparation video
03 / Burnout guidance
Match the program
to your flask.
Start in a room-temperature oven.
Flasks up to 3″ × 3″ (7.62 × 7.62 cm)
The time under each temperature is the hold at that temperature.
Swipe the chart to see the complete program →
| Target temperature | Time to reach target | Hold at target |
|---|---|---|
| 93 °C | ||
| 180 °C | ||
| 900 °C | ||
Cooling: no fixed duration is specified; follow the temperature required by your casting process.
Final hold by flask size
Final hold by flask size
| Flask size | Target temperature | Final hold |
|---|---|---|
| Flasks up to 3″ × 3″ (7.62 × 7.62 cm) | 900 °C | 3 h |
| Larger flasks | 900 °C | 4 h |
Your next casting
Let’s make every
detail count.
Discuss FERRO VEST V.H.T., your casting process or your next order with the PRESTIGE team.